Calcium Treatment: The Magic of Inclusion Modification
Al-killed steel is clean, but residual alumina (Al₂O₃) inclusions are a headache: hard, sharp, melting at 2050°C — solid particles in steel that clog nozzles during casting and form hard defects in slabs.
Calcium treatment is the magic fix: add Ca to turn solid sharp alumina into rounded liquid Ca-aluminate inclusions.
Principle
Ca + Al₂O₃ → CaO·Al₂O₃. Controlled Ca additions convert high-melting (2050°C) pure alumina into low-melting Ca-aluminates. 12CaO·7Al₂O₃ melts at ~1455°C — liquid at steel temperature. Liquid inclusions float out and don't build up on nozzles.
How to Add Ca
Ca boils at 1484°C — below steel temperature — so direct addition splashes violently. Industrial routes:
- Ca-Fe cored wire (wire feeding): Ca wrapped in steel shell, fed at 100~200 m/min deep into the ladle.
- CaSi alloy: with other alloys.
- Powder injection: argon carries Ca powder into the steel.
Wire feeding dominates — precise dosage, controlled speed and stirring.
Timing
After LF refining, before ladle release: measure temperature before feeding (too cold = poor Ca pickup); argon stir during; soft blow after to float modified inclusions. Success: better castability, no frequent nozzle clogging, acceptable inclusion rating.
Over-Calcium Problem
Excess Ca forms CaS, hurting properties, and extra Ca-aluminates. Dosage must be precise — "just enough to modify all Al₂O₃" — based on oxygen activity and sulfur content.
Summary
Calcium treatment is steel's transformation act: hard sharp high-melting inclusions become round liquid low-melting ones, improving castability and cleanliness. Every step relies on precise process control.