Metallography 101: From Grinding to Rating
Beyond chemistry, steel quality includes metallographic structure — grain size, ferrite/pearlite ratio, inclusion content. Metallography magnifies these structures for rating against standards.
Full Workflow
1. Sampling: representative location, 10~20mm, water-cooled cutting to avoid overheating.
2. Mounting: hot/cold mounting for thin or small pieces.
3. Grinding (patience!): P180→P400→P800→P1200→P2000, rotating direction each grade until previous scratches vanish. Everything depends on this.
4. Polishing: cloth + diamond paste until mirror-like, scratch-free.
5. Etching: e.g., 4% nital for steel, seconds — grain boundaries and phases etch preferentially. Too light: invisible; too deep: black.
6. Observation and rating: 100~500×, rate against GB/T 6394 (grain size), GB/T 10561 (inclusions).
What You See
- Grain size — finer = stronger (refinement strengthening)
- Structure type — ferrite, pearlite, martensite, austenite
- Ductile iron nodularity
- Inclusion rating — sulfides, oxides, silicates
- Decarburized/carburized layers
Fast Alternatives at Furnace Front
Classical sample prep takes 30+ minutes — too slow. Front-line options: thermal analysis cups (fast CE/nodularity inference); portable metallography for welds/large parts; fracture observation for quick structure checks. Fast methods find problems; lab metallography confirms.
Summary
Metallography is the internal exam of steel — grinding, polishing, etching, observing, rating. For quick foundry structure checks, thermal analysis and fracture observation are the fast lane.